University of Waikato Research
Permanent URI for this communityhttps://researchcommons.waikato.ac.nz/handle/10289/10288
Browse
3 results
Search Results
Item type:Publication, Factors controlling the tensile properties of ultrafine structured Cu–5vol%Al₂O₃ nanocomposite prepared by high energy mechanical milling and powder compact extrusion2013, ElsevierThe microstructures and tensile properties of two ultrafine structured Cu–5vol%Al₂O₃ nanocomposite samples made by a combination of high energy mechanical milling of a mixture of Cu powder and gamma Al₂O₃ nanopowder and powder compact extrusion were studied. The sample extruded at 750 °C exhibited a microstructure consisting of Cu grains with sizes in the range of 100–500 nm and a dispersion of Al₂O₃ nanoparticles with sizes in the range of 20–345 nm. With the extrusion temperature increasing to 900 °C, the Cu grain sizes remained almost unchanged, but a large fraction of the Al₂O₃ nanoparticles were dissolved, leading to possible formation of nanometer sized Al³⁺/O²⁻ clusters. This microstructural difference of the two samples causes an interesting difference in tensile properties, with the sample extruded at 900 °C showing approximately 150 MPa higher yield strength and ultimate tensile strength and also better ductility than the sample extruded at 750 °C. It appears that this significant beneficial effect of dissolution of Al₂O₃ nanoparticles is mainly caused by the significant strengthening effect of the nanometer sized Al³⁺/O²⁻ clusters through Orowan mechanism.Item type:Publication, Mechanical behaviour of ultrafine grained Cu and Cu-(2.5 and 5) vol.%Al₂O₃ composites produced by powder compact forging2011, Trans Tech PublicationsNanostructured Cu-(2.5 and 5) vol.%Al₂O₃ composite powders were produced from a mixture of Cu powder and Al₂O₃ nanopowder using high energy mechanical milling, and then compacted by hot pressing. The Cu and Cu- Al₂O₃ composite powder compacts were then forged into disks at temperatures in the range of 500-800°C to consolidate the Cu and Cu- Al₂O₃ composite powders. Tensile testing of the specimens cut from the forged disks showed that the Cu forged disk had a good ductility (plastic strain to fracture: ~15%) and high yield strength of 320 MPa, and the Cu-(2.5 and 5)vol.%Al₂O₃ composite forged disks had a high fracture strength in range of 530-600 MPa, but low ductility.Item type:Publication, Microstructure and mechanical behaviour of ultrafine grained Al-4wt%Cu-(2.5-10) Vol.% SiC metal matrix composites produced by powder compact forging2011, Trans Tech PublicationsUltrafine grained Al-4wt%Cu-(2.5-10) vol.% SiC metal matrix composite powders were produced from a mixture of Al, Cu and SiC powders using high energy mechanical milling (HEMM). The composite powders produced were first hot pressed at 300°C with a pressure of 240 MPa to produce cylindrical powder compacts with a relative density in the range of 80-94% which decreased with increasing the SiC volume fraction. Powder compact forging was utilized to consolidate the powder compacts into nearly fully dense forged disks. With increasing the volume fraction of SiC from 2.5% to 10%, the average microhardness of the forged disks increased from 73HV to 162HV. The fracture strength of the forged disks increased from 225 to 412 MPa with increasing the volume fraction of SiC particles from 2.5 to 10%. The Al-4wt%Cu-2.5vol.%SiC forged disk did not show any macroscopic plastic yielding, while the Al-4wt%Cu-(7.5 and 10)vol.% SiC forged disk showed macroscopic plastic yielding with a small plastic strain to fracture (~1%).